Influencing Factors Of Compression Cold Resistance Coefficient Of Cast Polyurethane Elastomer

Jul 28, 2025 Leave a message

Abstract In this study, polyols such as polytetrahydrofuran diol (PTMG), polyester diol (PEA, PBA), polycaprolactone diol (PCL), polycarbonate diol (PCDL), and polyphenylmethane diisocyanate (MDI), P-phenyldiisocyanate (PPDI), naphthalene diisocyanate (NDI) and other polyisocyanates and various chain extenders were used to synthesize cast polyurethane elastomers with similar hardness (Shao A hardness 94~96).Through systematic analysis, the following conclusions are revealed:

Soft section structure: The compression cold resistance coefficient of PTMG polyether elastomers is significantly higher than that of polyester (PCL, PCDL, etc.) because of its better ether bond compliance.

Molecular weight of the soft segment: When the molecular weight of PTMG increases from 1000 to 2900, the compression cold resistance coefficient tends to rise first and then fall, reaching a peak at Mn=2000.

 

Hard segment factors: The structural regularity of diisocyanate is sorted as PPDI ≈ NDI > TODI> MDI. The higher the regularity, the higher the compression cold resistance coefficient.The longer the molecular chain of the chain extender (such as HQEE containing a rigid benzene ring), the more conducive it is to improve the cold resistance coefficient.The increase in the content of the hard segment (such as the increase in the mass fraction of the prepomer NCO from 8.5% to 9.5%) leads to a decrease in the compression cold resistance coefficient.

 

Process optimization: The prepromerization method/semi-prepromerization method (high degree of micro-phase separation) is better than the one-step method.The low-temperature vulcanization process (80℃/72h) is more conducive to improving the compression cold resistance coefficient than the high-temperature vulcanization (120℃/8h).

 

1.Analysis of key influencing factors
1.1 The influence of soft segment structure
Polyether vs polyester: PTMG contains a large number of ether bonds (low free rotation resistance), and its elastomer compression cold resistance coefficient (0.43) is much higher than that of polyester type (such as PBA only 0.15), due to the large base of polyester esters, it is easy to crystallize at low temperatures.
1.2 Influence of molecular weight of soft segment
When the molecular weight of PTMG increases from 1000 to 2900, the compression cold resistance coefficient peaks at Mn=2000 (0.46).An increase in molecular weight will enhance the softness of the soft section, but too high (>2000) will cause crystallization and reduce athletic ability.
1.3 The impact of hard section structure

Diisocyanate type:

Diisocyanate Compression cold resistance coefficient Rebound rate (%)

MDI

0.43 55
PPDI 0.63 65
NDI 0.62 68
TODI 0.58 61

 

Conclusion: The rigid structure of PPDI/NDI promotes the regular arrangement of hard segments and significantly improves cold resistance.

 

Type of chain extender:

Chain extender Compression cold resistance coefficient
BDO 0.43
HDO 0.46
HQEE 0.52
DEG 0.18

 

Conclusion: The chain extender containing rigid structures (such as the benzene ring of HQEE) can enhance the micro-phase separation, while the DEG ether bond destroys the density of the hard zone.

 

Hard segment content: The NCO mass fraction of the prepomer increased from 8.5% to 9.5%, the proportion of the soft segment decreased, the compression cold resistance coefficient decreased from 0.48 to 0.35, and the hardness increased from 94A to 96A.

 

1.4 The influence of the preparation process
Synthesis method: The compression cold resistance coefficients of the one-step method, the semi-prepromer method, and the prepromer method are 0.38, 0.44, and 0.43, respectively.The prepromerization method promotes micro-phase separation and optimizes low temperature performance.
Vulcanization process: low-temperature vulcanization (80℃/72h, coefficient 0.47) is better than high-temperature vulcanization (120℃/8h, coefficient 0.38), which promotes the crosslinking reaction to generate urea formate bonds due to high temperature, reducing the degree of micro-phase separation.

2. Conclusion


Soft segment optimization: PTMG with Mn=2000 is preferred as the soft segment substrate.
Hard section design: Choose high-regularity diisocyanates such as PPDI/NDI, and use HQEE chain extender.Process control: The prepromer method is used in combination with the 80℃/72h vulcanization process to maximize the compression cold resistance coefficient.